Episode 5: BioPin's Inspection Standards During Carbon Coating Process Stage

November 02, 2026
Anhui BIOPIN IOT Group
A reliable supplier of New Energy Battery Aluminum Materials product .
Anhui BIOPIN IOT Group

In this issue, BioPin will introduce the inspection standards for the carbon coating process stage. There are three different sampling frequencies.

 

1. 1 Time/ 3 Rolls/ Processing Step (Number of Inspections Per Volume: 3; Take the Average Value)

Inspection Norm Including :

1) Burrs and Indentation

Using optical microscope, the sample length at the end of the roll is approximately 1.5 meters. with a standard of Rip length ≤ 50 μm, ≤ 10 features per 500 mm spacing; spacing greater than 50 m; notch depth ≤ 8 μm; ≤ 5 features per 500 m spacing; spacing greater than 100 m

2) Foil Thickness 

Using a digital micrometer(0.0001), perform uniform sampling along the width direction within the photofoil region according to the sample size, with a standard of base aluminum foil’s thickness ± 0.5 μm (refer to the process specifications for further details).

3) Foil Surface Density

Using an electronic balance and a quantitative sampler, perform uniform sampling along the width direction within the photofoil area according to the specified sample quantity, with the standard of  32.5±1.6g/m²(12μm bare aluminum foil)  or35.23±1.5g/m²(13μmbare aluminum foil) (refer to the process standards for further details).

4) Foil Width

Using a film ruler, perform uniform sampling along the width direction within the photofoil area according to the specified sample quantity, with a tolerance of ±0.5 m (refer to the process standards for specific details).

5) Coating Width

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.5 mm (refer to the process standards for specific details).

6) Blank Space Width in the Middle of the Aluminum Foil

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.5 m (refer to the process standards for specific details).

7) Blank Space Width on Both Side Edges

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.8 m(refer to the process standards for specific details).

8) Registration Accuracy

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ≤0.8 mm (refer to the process standards for specific details).

9) Coating Medium State

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ≤0.8 mm (refer to the process standards for specific details).

10) Length of Intermittent Coating

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.5 m (refer to the process standards for specific details).

11) Blank Space of Intermittent Coating

Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.5 m (refer to the process standards for specific details).

12) Surface Density

Using an electronic balance, quantitative sampler, and heat gun, perform uniform sampling along the width direction within the photofoil area according to the specified sample quantity, with a standard of 33.5±1.5g/m²(12μm mill finished aluminum foil)35.86±1.6g/m²(13μm mill finished aluminum foil)(refer to the process standards for further details).

13) Total Thickness

Using a digital micrometer(0.0001), perform uniform sampling within the measurement area according to the sample size, with a standard of (base aluminum foil’s thickness+2μm )±0.8  (refer to the process standards for specific details).

14) Coating Density(Double Sides)

Using an electronic balance, quantitative sampler, and heat gun, perform uniform sampling along the width direction within the photofoil area according to the specified sample quantity, with a standard of 0.7±0.2 g/m²(refer to the process standards for further details).

 

2. 1 Time/ 3 Rolls/ Processing Step (Number of Inspections Per Volume: 5; Take the Average Value).

Inspection Norm Including :

1) Tensile Strength

Using a sample holder (15 mm) and a tensile testing machine, feed flat samples measuring approximately 15 m × 150 m, with a standard value of ≥230 MPa (refer to the specific process standards for further details).

2) Elongation

Using a sample holder (15 mm) and a tensile testing machine, feed flat samples measuring approximately 15 m × 150 m, with a standard value of ≥2.5% (refer to the specific process standards for further details).

 

3. Full Inspection

Inspection Norm Including :

1) Roll Length

Check using a meter.

 

Quality control at the carbon coating stage is critical to the final performance of carbon-coated aluminum foil. By following this set of inspection standards, we can reliably manage defects. In our next episode, BioPin will bring you another quality inspection standard related to battery foil production.

Latest Blog
inquiry_img
Leave A Message
If you are interested in our products and want to know more details,please leave a message here,we will reply you as soon as we can.

leave a message

leave a message
If you are interested in our products and want to know more details,please leave a message here,we will reply you as soon as we can.
Contact Us: peng@biopin.vip

home

products

WhatsApp

Contact Us