In this issue, BioPin will introduce the inspection standards for the raw material input stage (including aluminum foil raw materials and slurry raw materials).
Part 1:Aluminum Foil Raw Materials Inspection
In this part, the sampling frequency is as follows: one sample is taken from each master roll; for each batch of precision-cut finished rolls, 10% of the roll count is sampled, and each sampled roll is inspected three times, with the average value taken.
Inspection Norm Including :
1) Foil Width
Using a film ruler, perform uniform sampling within the measurement area according to the sample size, with a tolerance of ±0.5 mm (refer to the process standards for specific details).
2)Foil Thickness
Using a 0.01 mm ruler, perform uniform sampling along the width direction within the photofoil region according to the sample size, with a standard of h ± 0.5 μm (refer to the process specifications for further details).
3)Foil Density
Using an electronic balance and a quantitative sampler, perform uniform sampling along the width direction within the photofoil area according to the specified sample quantity, with a tolerance of ±5% relative to σ (refer to the process standards for further details).
4)End Face
Using a light microscope, the sample length at the end of the roll is approximately 1.5 meters. The inspection criteria are as follows: burr length ≤ 50 μm and ≤ 10 burrs per 500 mm interval; for intervals exceeding 500 mm, burr length ≤ 50 μm and ≤ 5 burrs per 500 mm interval; notch depth ≤ 8 μm and ≤ 5 notches per 500 mm interval; for intervals exceeding 100 mm, notch depth ≤ 8 μm and ≤ 5 notches per 500 mm interval.
5)Tensile Strength
Using a sample holder (15 mm) and a tensile testing machine, feed flat samples measuring approximately 15 m × 150 m, with a standard value of ≥230 Pa (refer to the specific process standards for further details).
6)Elongation
Using a sample holder (15 mm) and a tensile testing machine, feed flat samples measuring approximately 15 m × 150 m, with a standard value of ≥2.5% (refer to the specific process standards for further details).
7)Pinhole
When using a pinhole box, for widths ≤500 m, sampling and measurement shall be performed across the entire width; for widths>500 m, measurements shall be conducted in two equal portions, adhering to the following testing standards: offline testing: for pinholes with diameter ≤0.3 mm, the number of pinholes shall be ≤5 per m²; for pinholes with diameter>0.3 mm, no defects are permitted.
8) Plate Shape
Testing performed using an offline sheet thickness gauge; parameter settings: coiling tension stress = 0.8 kgf/mm²—full-width measurement. There are two inspection criteria: one is that the collapse width at the midpoint of the coil shall not exceed 0.6 mm (no requirement for collapse width); alternatively, if the collapse width is between 0.6 mm and 0.8 mm and the collapse width range does not exceed 100 mm, the product shall be deemed qualified; otherwise, it shall be deemed unqualified. Another is that the difference in collapse width between the two edges of the coil (edge collapse) shall not exceed 0.6 mm.
Part 2:Slurry Raw Materials Inspection
Based on the frequency of inspection, the inspection items are primarily divided into two categories.
Firstly, the sampling frequency is to perform one inspection per batch, sampling 10% of the incoming material (by number of barrels), with a minimum sample size of one barrel.
1) Binder
a.Viscosity
Using a rotating viscosimeter. Use 500–600 ml of raw material, η±500mPa·s (refer to the specific process standards for further details); η denotes viscosity.
b.Solid Content
Using a Halogen Moisture Analyzer (physical analysis method, drying), use 2~3g of raw material, wt±1.0 % (refer to the specific process standards for further details); wt denotes solid content.
c.PH Value
Using a PH meter. Use 500ml of raw material, p±1 (refer to the specific process standards for further details). P denotes PH.
Secondly, the sampling frequency is to perform conductive sampling inspections on 10% of the incoming materials per quarter (by case/bag), with a minimum of 1 case/bag.
Inspection Norm Including :
1) Conductive Agent
a.Moisture Content
Using a Karl Fischer Moisture Analyzer (Chemical Reaction Analysis), use 50 g of raw material (Carbon black): ≤0.5%; (Graphite): ≤0.5%.
b.Ash Content
Using a muffle furnace and analytical balance. Use 50 g of raw material: (Carbon black): ≤0.1%; (Graphite): ≤1%.
c. Specific Surface Area
Using a Fully Automated Specific Surface Area and Pore Size Analyzer. Use 50g of raw material: (Carbon black):20-70m²/g ; (Graphite): 10-60m²/g.
d. Elemental Impurities
Using an Atomic Absorption Spectrometer. Use 50g of raw material: (Carbon black): Fe≤20、S≤500ppm; (Graphite): Fe < 200 ppm.
2) Alkaline Agent(purity)
Using a burette, potentiometric titrator, and electronic analytical balance, use 0.5g of raw material. The testing criterion is purity> 98%.
3) Wetting Agent (purity)
Using a gas chromatograph, use 10ml of raw material; the testing criterion is Alcohol content ≥ 99.9%, moisture content ≤ 0.20.
Part 3: Auxiliary Material Inspection
Based on the frequency of inspection, the inspection items are primarily divided into three categories.
Firstly, the sampling frequency of conducting sampling inspections is full inspection(100%).
Inspection Norm Including :
1) Roller
Using Film Strip Roundness Tester, Sample and test per root, Tolerance and round runout (refer to the process standards for specific details).
2) Rubber-Covered Roller
Using Film Strip Roundness Tester, Sample and test per root, tolerance, roughness, and round runout (refer to the process standards for specific details).
Secondly, the sampling frequency of perform Conduct sampling inspections is for each batch of incoming materials; sample 10% of the quantity (boxes), with a minimum of 3 tablets per box.
Inspection Norm Including:
1)Blade
Using a 2.0D measurement machine, Sampling and testing by sheet, Gap (refer to the process standards for specific details).
Thirdly, the sampling frequency of conducting sampling inspections is: for each batch of incoming materials, sample 10% of the quantity, with a minimum sample size of 1 unit.
Inspection Norm Including:
1) Wooden Box
Using a film ruler, Sample and test one unit at a time. Tolerance range (refer to the process standards for specifics).
2) Tube Core
Using a film ruler, Sample and test per root. Tolerance range (refer to the process standards for specifics).
3) EPE Foam
Using tape, sampling and testing by sheet, Thickness (refer to the process standards for specifics).
4) Aluminum-Plastic Film Bag
Using 10,000ths of a meter, sampling and testing one unit at a time, Thickness (refer to the process standards for specifics).
5) Drying Agent
Using a moisture analyzer, Sampling and testing by batch, Moisture (refer to the process standards for specifics).
Above all are all the incoming material inspection norms and related inspection standards. In the next blog, we will continue to share BioPin’s other inspection norm details. We look forward to your anticipation.